Specifications

4 5
1 2 3
REPAIR OF KÄHRS WOOD FLOORS
GLUING OF UNLOCKED WOODLOC 5S JOINTS
In case of an unlocked Woodloc 5S joint, this is a simple way
of rectifying the problem.
1. Mark at the tounge side of the board according to picture.
2. Drill 1012 mm depth into the board. Note, the drilling depth
is important, you have to drill in order to reach the cavity
(see picture 4).
3. Lift up the board using a suction cup.
4. Inject glue into the drilled holes while continuing lifting the
board.
5. Put pressure immediately after injecting glue. Maintain
pressure for at least 3 minutes.
Repair the drilled holes using Kährs meltable filler sticks.
Recommended glue: Loctite 3090