Data Sheet

TEXTURE FORMING:
The “spattered texture” is the result of 2 coatings which are ap -
plied in a sequence of 15 – 20 minutes* between the base and
the spattered coating:
I. CONDITIONS FOR THE BASE COATING:
Nozzle diameter: 0,078 inch 2,0 mm
Airpressure: 28 – 57psi 2 – 4 bar
Materialpressure: 28 – 71 psi 2 – 5 bar
Spraying Distance: 1 ft 30 cm
II. CONDITIONS FOR THE SPATTERED COATING:
Nozzle diameter: 0,078 inch 2,0 mm
Airpressure: 7 – 21psi 0,5 – 1,5 bar
Materialpressure: 28 – 71 psi 2 – 5 bar
Spraying Distance: 1,3 ft 40 cm
VARIATION OF TEXTURE FINISH:
parameter te
air pressure low / high big dots / small dots
material pressure higher smoother surface
spraying distance with larger range rough and more pointed
more cross coats closer
DRYING / FORCED DRYING:
At room temperature:
dust free = 15 – 20 minutes *
ready for handling = 2 – 3 hours *
ready for packing = 1 day *
through dry = 4 days *
Oven drying:
Coated substrates may be heated at elevated temperatures
of approx. 60°C to speed up drying process.
y,
air circulation, condition of the surface.
WARNEX:
enhancing textures