Approval/Certificate/Document of Conformity

BS EN ISO 4589-2: 1999
Appendix A
MATERIAL TESTED
Part 1 - Preliminary oxygen concentration
Oxygen Concentration (%)
35.0 38.0 36.0
Burning Period (s)
32.5 177.5 >180
Length Burnt (mm)
<10 >50 40
Response (‘X’ or ‘O’)
O X X
Part 2 - Determination of the oxygen index value
N
T
series measurements
N
L
series measurements (8.5)
(8.6.2) C
f
Oxygen
Concentration (%)
35.0 35.2 35.4 35.4 35.2 35.0 35.2 35.0
Burning Period (s) 39 57 >180 >180 >180 42 >180 47.5
Length Burnt (mm) 10 10 30 30 40 10 25 10
Response
(“X” or “O”)
O O X X X O X O
Column (2,3,4 or 5) 3 Row (1 to 16) 11
k value from table 4 0.94
Hence k = 0.94
Oxygen index value OI = C
F
+ kd
d is oxygen concentration increment
OI = 35.0 + (0.94 x 0.2)
Oxygen index value = 35.2 (to one decimal place for reporting)
= 35.19 (to two decimal places, for calculation of and verification
of d as required in Part 3)
Standard Deviation = 0.15 Therefore, the test result is valid.
Part 3Burning characteristics of the material
No
relevant ancillary characteristics or behaviour such as, charring, dripping, severe shrinkage, erratic
burning, or after-glow were observed during the test.
Document No.: Additional Test Report 386711 Page No.: 7 of 8
Author: T. Mort Issue Date: 28
th
July 2017
Client: Weidmüller Interface GmbH &
Co. KG.
Issue No.: 1